time and additives on the alkali content of coal-cinder from the catalytic gasification of pulverized anthracite were examined by using the static calcination method in a laboratory high temperature furnace in this study.The results indicated that the optimum calcination temperature and time were respectively 870℃and 30 min
and the optimum dealkalization additive is kaolinite.By adding only 5% kaolinite in the calcination process
the dealkalization rate could be increased to 100%.Most importantly
with analyzing the calcined cinder by X-ray powder diffraction (XRD) and scanning electron microscope(SEM)
it was clear that at an appropriate calcination temperature
the activated SiO2 and Al2O3 in alkaline coal-cinder would react with the decomposed fused Na2CO3 to form a new neutral matter nepheline(NaAlSiO4)and other amorphous silicate compounds
causing an obvious reduction of the alkali content in coal-cinder.